Just used a batch of Tamiya acrylics for a color that is not in their range. Thinned with Mr Leveling thinner, sprayed through Iwata HP-CS w/.3 needle, compressor at 20 lbs pressure.
Paint covered well but all surfaces were left with an almost “pebbly” finish, rough to the touch.
I’m going to let the parts set for two days before trying any recommended fix. I have experienced similar issue before, resolving it using fine sanding, which I’m concerned would end up burning through to the plastic. I believe I read in the past that spraying the rough areas with straight thinner would smooth the surface. Not sure, and heck, that’s why I’m posting for your ideas, experiences and recommendations.
Is the paint going on wet? Sounds like the paint is drying on contact and thus not leveling as it would if applied wet. Not so wet that it puddles or runs.
If you aren’t using the paint manufacturer’s recommended thinner you should not be surprised when you have problems using the paint.
What you are describing as “pebbly” sounds much worse than the common “sandpapery” finish people get when Tamiya acrylics aren’t thinned enough (*). The latter generally goes away with another coat of well-thinned paint; not sure if that will be enough for the former texture.
(*) “Enough” depends on the solvent remaining in the paint, humidity, air pressure, nozzle type, and spraying distance. Adjusting those other parameter will often make Not Enough become Enough.
KL
What you are getting is severe orange peel verging into dusting. You didn’t specify the thinning ratio, which is critical. Thin Tamiya X and XF paints either with their proprietary thinner, which contains a retarder, or with 90% isopropyl alcohol with a few drops of Tamiya or other acrylic retarder. Thin at a ratio of approximately 1:1. Drop your air pressure to 14-15 psi. 20 psi is way too high.
You also didn’t mention temperature and humidity. Both affect Tamiya X and XF paints. If it is over 70°F, the thinner and retarder should be increased. Low humidity the same. High humidity requires multiple, thin coats.
And the paint should have a wet sheen on the surface immediately after application.
I have had this happen and sprayed over with a thin coat of MLT and it went away.
Normally your mixture and settings are nearly perfect for an excellent result. Pebbling is a frequent mishap in airbrushing. It results from the paint drying on the way to the model, before it hits the surface. You need to drop your PSI a little (15 PSI) and get closer to the model with the airbrush. This should give you a perfect finish.
I’ve heard of guys fixing pebbling with a coat of straight MLT, but have never tried it myself. I guess trying it is better than stripping the paint and starting over.
Not the case with Tamiya Acrylics, especially with MLT. My guess is your air pressure is too high, reduce to 15 psi and try that.
What’s not the case with Tamiya acrylics - that using a non-recommended thinner is guaranteed to be trouble free? Why risk it?
I think most problems can be solved by controlling and adjusting the known factors affecting performance (paint consistency, thinner ratio, temperature/humidity, and air pressure) rather than introducing something else that may not work next month or with an older bottle of paint.
KL
Kurt, I’ve used Lacquer thinners with Tamiya Acrylic based paints for years. I have used both Tamiya Lacquer thinner and MLT with fantastic results. Just my 2 cents man, you paint whatever way works for you.
In this case though, things weren’t working for the OP, and he asked for help.
It’s always harder to troubleshoot when things aren’t set up the way they are intended to be. I won’t say using MLT caused this guy’s problem, but it clearly didn’t prevent it either. Thinning more and changing air pressure are thinner-independent (to an extent), so it’s worth the OP asking himself why he’s using it in the first place.
KL
My thanks to all who responded with comments/recommendations. As the paint had hardened, I used 3600/5000/6000 sanding to drop back to a smooth finish, which I will re-approach with the information y’all have shared. Regarding the thinning ratio, this was done by eye, not by measurement, and continued mixing in trying to arrive at the right color (CARC Sand, BTW).
I live in the Mojave desert, low humidity and temps usually in 80-90 F range, but air conditioning keeping temps inside as a decent level. Next time around I will use the proprietary thinner for the paint used, and drop the pressure below the usual 20 psi.
Thanks again!